  • Fused cast AZS brick 41 for glass furnace

Fused cast AZS brick 41 for glass furnace

Catalog: Fused cast AZS 41 | 2016-01-15

Model Number:AZS 33-36-41
ZrO2:32-44%
Bulk Density:3.7-4.1g/cm3
Cold Crush Strength:350MPa

Product Details

Oxidation fused-cast zirconia-corundum Products

He144a174e480418292e4294f1d71ad5fZ.png

The fused zircon corundum brick is a white solid formed by pure alumina powder and zircon sand containing zirconia of 65% and about 34% of silica in the electric melting furnace and then injected into the mold to be cooled.

Zircon brick / Zirconia bricks have the advantage of mechanical strength, excellent stability to thermal shock, resistance to
corrosion, high refractorines
s under load and inertness, high density, etc. It is widely used in glass furnace, non-ferrous metal smelting furnace, and pure steel furnace. Please see listed applications on lower right of this page.
TK BRICKS can produce serious fused cast 33#,36#,41#AZS block for glass furnace.

We can produce common shaped and irregular shaped refractory brick.And we can adjust our specifications for your application.
Specification

ITEM
SPEC
AZS-33#
ER 1681
AZS-36#
ER 1685
AZS-41#
ER 1711


Chemical
Composition
Al2O3
≥50.00
≥49.00
≥45.00
ZrO2
≥32.50
≥35.50
≥40.50
SiO2
≤15.50
≤13.50
≤13.00
Na2O+K2O
≤1.30
≤1.35
≤1.30
Bulk density g/cm3
≥3.75
≥3.85
≥4.00
Apparent Porosity %
≤1.2
≤1.0
≤1.2
Cold Crushing Strength Mpa
≥300
≥300
≥300
Exudation Temperature of Glass Phase
≥1400
≥1400
≥1410
Bubble Separation Ratio(1300°C×10h)
≤1.2
≤1.0
≤1.0
Anti-corrosion rate of glass liquid
1500°C×36h (mm/24h)%
≤1.4
≤1.3
≤1.2

Apparent density
(g/cm3)
PT(RN RC N)
≥3.50
≥3.50
≥3.70
ZWS(RR EVF EC ENC)
≥3.65
≥3.70
≥3.90
WS( RT VF EPIC FVP DCL)
≥3.75
≥3.8
≥4.00

He3f9017b60294f518edea5775ef7afd1g.png